CAD/CAM technology is one of the fastest growing areas of digital restorative dentistry. The aim of the study was to evaluate in vitro the effect of glazing and thermocycling on the microhardness of ceramic veneers under the assumption that there is a significant difference between the microhardness values of different glazed and unglazed CAD/CAM materials.Materials and methods.
The microhardness of 80 veneer specimens from four different ceramic CAD/CAM materials were measured: 1) IPS E.max CAD lithium disilicate ceramic (Ivoclar, Germany); 2) IPS Empress CAD leucite glass ceramic (Ivoclar); 3) Cerec feldspathic ceramic (Dentsply Sirona, Germany); and 4) Cerasmart hybrid ceramic (GC, Japan). All specimens were divided into 4 equal groups, and in each group, half (10) of the veneers were glazed. All veneer specimens were subjected to 10,000 thermocycles to simulate one year of service. Vickers microhardness values were measured at three stages: after milling, after glazing, and after thermocycling. SEM images of the surface of the samples after milling and after thermocycling were also obtained.
Results.
Statistically significant differences between microhardness values of different materials after glazing and thermocycling were revealed. Microhardness values after glazing decreased by 5% for E.max, by 7—9% for Empress and Cerec, and by 34% for Cerasmart. E.max specimens showed higher microhardness values after glazing (601±13 MPa) compared to Empress (575±12 MPa), Cerec (453±16 MPa), and Cerasmart (76 MPa; p<0.05). Glazed surface analysis also revealed statistically significant differences after thermocycling (p<0.05). Tamhein's T2 post hoc test confirmed that the microhardness values of the E.max group were significantly higher after thermocycling compared to the Cerasmart, Empress and Cerec groups (p<0.05). The effect of thermocycling was also evident for unglazed samples where the E.max group showed higher microhardness values (641±7 MPa) compared to Cerasmart, Empress and Cerec groups (p<0.05).
Conclusion.
Glazing and thermocycling reduced the microhardness of veneers made of the investigated materials. E.max and Empress samples showed the highest microhardness of about 600 kgf/mm2. Comparable values of about 500 kgf/mm2 were shown by Cerec feldspathic ceramics. The microhardness of Cerasmart samples was much lower, in the order of 100 kgf/mm2 (p<0.05). The study highlights the importance of glazing and thermocycling in evaluating the microhardness values of ceramic CAD/CAM materials, revealing the peculiarities of their behavior in clinical use. Thermocycling did not significantly decrease the microhardness.
Key words:
CAD/CAM ceramic blocks, restorative and digital dentistry, feldspathic ceramics Cerec, leucite reinforced ceramic Empress, hybrid ceramic Cerasmart, lithium disilicate E.max.For Citation
[1]
Ahmedbeyli F.R., Ahmedbeyli R.M., Ersoy M. The effect of glazing and thermocycling on microhardness of different milled ceramic laminate veneers with SEM observations. Clinical Dentistry (Russia). 2024; 27 (3): 45—50. DOI: 10.37988/1811-153X_2024_3_45
References
- Spitznagel F.A., Boldt J., Gierthmuehlen P.C. CAD/CAM Ceramic restorative materials for natural teeth. J Dent Res. 2018; 97 (10): 1082—1091. PMID: 29906206
- Sevbitov A.V., Brago A.S., Enina Yu.I. Experience in the application of hybrid ceramic restorations in the cervical region. Clinical Dentistry (Russia). 2017; 3 (83): 10—12 (In Russian). eLIBRARY ID: 29960527
- Panahov N.A., Aliyeva S.S. The results of using CAD/CAM-made zirconium crowns. Clinical Dentistry (Russia). 2019; 2 (90): 76—79 (In Russian). eLIBRARY ID: 37749530
- Kömürcüoğlu M.B., Sağırkaya E., Tulga A. Influence of different surface treatments on bond strength of novel CAD/CAM restorative materials to resin cement. J Adv Prosthodont. 2017; 9 (6): 439—446. PMID: 29279763
- Goryainova K.E., Rusanov F.S., Poyurovskaya I.Ya., Retinskaya M.V., Lebedenko I.Yu. Comparative assessment of strength of dental CAD/CAM materials for chairside techniques. Russian Journal of Dentistry. 2016; 3: 116—120 (In Russian). eLIBRARY ID: 26331214
- Nguyen J.F., Migonney V., Ruse N.D., Sadoun M. Resin composite blocks via high-pressure high-temperature polymerization. Dent Mater. 2012; 28 (5): 529—34. PMID: 22230107
- Nguyen J.F., Migonney V., Ruse N.D., Sadoun M. Properties of experimental urethane dimethacrylate-based dental resin composite blocks obtained via thermo-polymerization under high pressure. Dent Mater. 2013; 29 (5): 535—41. PMID: 23522657
- Carrilho Baltazar Vaz I.M., Pimentel Coelho Lino Carracho J.F. Marginal fit of zirconia copings fabricated after conventional impression making and digital scanning: An in vitro study. J Prosthet Dent. 2020; 124 (2): 223.e1—223.e6. PMID: 32336539
- Zaruba M., Mehl A. Chairside systems: a current review. Int J Comput Dent. 2017; 20 (2): 123—149. PMID: 28630955
- Arezoobakhsh A., Shayegh S.S., Jamali Ghomi A., Hakimaneh S.M.R. Comparison of marginal and internal fit of 3-unit zirconia frameworks fabricated with CAD-CAM technology using direct and indirect digital scans. J Prosthet Dent. 2020; 123 (1): 105—112. PMID: 30982618
- Marti A.M., Harris B.T., Metz M.J., Morton D., Scarfe W.C., Metz C.J., Lin W.S. Comparison of digital scanning and polyvinyl siloxane impression techniques by dental students: instructional efficiency and attitudes towards technology. Eur J Dent Educ. 2017; 21 (3): 200—205. PMID: 26960967
- Zimmermann M., Mehl A., Mörmann W.H., Reich S. Intraoral scanning systems — a current overview. Int J Comput Dent. 2015; 18 (2): 101—29. PMID: 26110925
- Ahmed K.E. We’re Going Digital: The Current State of CAD/CAM Dentistry in Prosthodontics. Prim Dent J. 2018; 7 (2): 30—5. PMID: 30095879
- Blatz M.B., Conejo J. The current state of chairside digital dentistry and materials. Dent Clin North Am. 2019; 63 (2): 175—197. PMID: 30825985
- Goujat A., Abouelleil H., Colon P., Jeannin C., Pradelle N., Seux D., Grosgogeat B. Marginal and internal fit of CAD-CAM inlay/onlay restorations: A systematic review of in vitro studies. J Prosthet Dent. 2019; 121 (4): 590—597.e3. PMID: 30509548
- Gale M.S., Darvell B.W. Thermal cycling procedures for laboratory testing of dental restorations. J Dent. 1999; 27 (2): 89—99. PMID: 10071465
- Zaniboni J.F., Silva A.M., Alencar C.M., Porto T.S., Jasinevicius R.G., Fortulan C.A., de Campos E.A. Influence of different glaze firing protocols on the mechanical properties of CAD-CAM ceramic materials. J Prosthet Dent. 2022; 127 (6): 925.e1—925.e8. PMID: 35469648
- Çakmak G., Subaşı M.G., Sert M., Yilmaz B. Effect of surface treatments on wear and surface properties of different CAD-CAM materials and their enamel antagonists. J Prosthet Dent. 2023; 129 (3): 495—506. PMID: 34301415
Downloads
Received
April 9, 2024
Accepted
July 21, 2024
Published on
October 2, 2024